Staple Yarn Preparation: Ginning, Blowroom, Carding, Drawing and Combing
2. Principles of opening, cleaning and blending
Opening reduces large compressed tufts to small ones; cleaning removes trash (leaf, seed-coat, dust) from them; blending mixes bales so that the product is uniform. The three are linked: trash is locked inside tufts, so cleaning can proceed only as far as opening has gone. A beater strikes a tuft held or carried by an air stream; the tuft is flung against grid bars, and heavy trash falls through the gaps while fibres are carried on. Dust is drawn away by suction. Cleaning efficiency is defined as
cleaning efficiency (%) = (trash % in feed − trash % in delivery) ÷ (trash % in feed) × 100.
- Beater speed and type: a pin or spiked beater opens gently; a blade beater cleans more strongly but damages more. Higher speed and closer settings clean more and also raise fibre breakage and neps.
- Blending is done by mixing bale-by-bale (bale plucking from many bales at once) and by layering in a hopper or multi-mixer so that fibre properties are averaged. Blend proportion is by mass.
3. Modern blowroom machines
A modern blowroom is a chain of machines joined by pneumatic ducts, with gentle action first and stronger action later, so that tufts are already small when the strongest beaters meet them.
| Stage | Function |
|---|---|
| Automatic bale opener (plucker) | A travelling head takes thin layers of tufts from many bales; gives bale-wise blending |
| Metal and heavy-part trap | Magnets and detectors protect the card clothing from tramp metal |
| Mixer or blender | Long-term mixing and a buffer between stages |
| Pre-cleaner and fine opener | Beater and grid cleaning in one or more steps; heavy trash and dust removal |
| Foreign-matter detector or separator | Optical or sensor detection of coloured or polymer contamination, removed by an air jet |
| Chute feed to cards | Delivers tufts into a feed chute at each card; the column density sets the card feed and enables levelling |
Developments include fewer machines in the line (shorter line means fewer neps), automatic control of waste removal, cleaning intensity set by the amount of trash, and the replacement of the lap by direct chute feeding.
4. Carding: action, machine, setting and clothing
Carding opens tufts into individual fibres, removes remaining trash, short fibre and neps, partly parallelises fibres and delivers a continuous sliver. The carding action occurs where two wire-covered surfaces move at different speeds with their points facing each other (point-against-point): fibres are held on the slower surface and combed by the faster. The stripping action occurs when the points lean the same way and the faster surface lifts fibres off the slower one; the cylinder strips the taker-in in this way. The slow doffer collects fibres from the fast cylinder as a thin web, which is condensed into the sliver.
A conventional card is a roller-and-clearer or revolving-flat card with a feed lap and slower production. A modern card has a chute feed, extra pre-carding and post-carding segments (stationary flats and carding elements), a wider and faster cylinder, higher doffer speed and autolevelling; it delivers several times the production at equal or better sliver quality. The flats (a slowly moving chain of clothed bars) do most of the carding against the cylinder and carry away flat strips containing short fibre, trash and neps.
- Card setting is the gauge distance between surfaces, set with feeler gauges: feed plate–taker-in, taker-in–cylinder, cylinder–flats, cylinder–doffer. The settings are only fractions of a millimetre and differ from one pair of surfaces to another. A closer cylinder–flats setting raises carding intensity and neps removal but cuts more fibre and wears the wire faster.
- Card clothing is the wire on the working surfaces. Flexible clothing is saw-tooth or needle wire set in a fabric foundation (flats, and in older cards cylinder and doffer); metallic clothing is a continuous saw-tooth strip wound on a roller (taker-in, and cylinder and doffer in modern cards). Key parameters: tooth angle (a more acute, aggressive tooth grips fibre firmly but strips poorly), points per unit area (finer fibres need denser, finer wire), tooth depth and height. Sharp, undamaged teeth are essential, so clothing is ground.
5. Card sliver: periodic variation, autoleveller and production
Periodic mass variation repeats at a fixed length. A mechanical source (an eccentric or bent roller, a worn gear) delivers a fault once per revolution. The material delivered by a faulty roller of diameter d in one revolution is πd long. If the material is further drafted by a draft D between that roller and the delivery, the wavelength in the delivered sliver is
λ = π d × D. Example: a roller of 28 mm diameter with a draft of 6 after it gives λ = π × 28 × 6 ≈ 528 mm. A peak in the spectrogram at that wavelength points at that roller; a broad hill at a wavelength set by the fibre length, not by any roller, is a drafting wave instead, caused by floating fibres.
A card autoleveller corrects the mass of the sliver by changing the draft. In an open-loop system the mass is sensed at the feed (for example the density of the chute column or the feed thickness) and the feed-roller speed is altered after a delay equal to the distance from sensing to correction divided by the material speed; it cannot see its own errors. In a closed-loop system the mass is sensed at the delivery and fed back; it corrects its own drift but acts on material already made. Card levellers correct long and medium wavelengths, not short ones. Production: kg/h = delivery speed (m/min) × sliver tex × 60 ÷ 10⁶ × efficiency; at 120 m/min, 4800 tex and 90 % efficiency this is 31.1 kg/h. Draft = feed tex ÷ delivery tex, ignoring waste.
6. Roller drawing and the drawframe
Roller drafting attenuates a strand by passing it between roller pairs whose surface speeds rise in sequence. Draft = V_front ÷ V_back = (feed tex) ÷ (delivered tex), for no loss. A drawing machine usually creates a break draft (small, to prepare fibres) before the main draft. Several slivers are fed together (doubling, n), so delivered tex = n × feed tex ÷ draft. Doubling averages out irregularity: for independent random errors the CV of the doubled sliver falls by √n. A drawframe that uses 6 slivers of 3600 tex at draft 7.5 delivers 6 × 3600 ÷ 7.5 = 2880 tex.
Fibres gripped by neither roller pair are floating fibres; they move erratically and create drafting waves, so the roller setting (nip to nip) is set a little more than the longest fibre in the main zone, and kept small enough that short fibres are still controlled. Pressure bars, aprons or pins add control inside the zone. Common arrangements include three-over-three and four-over-three drawframe drafting with a weighted pressure bar, and double-apron drafting for roving and ring frames. Periodic variation in drawn sliver has the same two origins as in the card: mechanical (λ = πd × D) and drafting waves.
The drawframe autoleveller senses the input sliver mass (usually with a pair of grooved scanning rollers), a controller computes the correction, and a servo motor changes the main-draft speed at the instant the sensed material reaches the draft zone. The time lag is distance ÷ feed speed: with sensing 0.30 m ahead and a sliver speed of 15 m/min the delay is 0.30 ÷ 15 = 0.02 min = 1.2 s. It cures short, medium and long-term errors in the feed; closed-loop sensing on the delivery is used in addition on some machines.
7. Cotton combing
Combing removes short fibres (below a set length), neps and fine trash, and straightens fibres, so the noil is rejected: noil % = noil mass ÷ feed mass × 100. It makes finer, stronger, more even and cleaner yarns from long-staple cotton, at the price of lost fibre and a few extra machines (sliver-lap, ribbon-lap and comber). The cycle in each nip has four main stages.
- Feeding: the lap is fed forward a small amount per nip (feed per nip, a few millimetres) to the nippers.
- Nipping and combing: the nippers close on the fibre fringe and the half-lap, a needle-covered segment of the rotating cylinder, combs the protruding fringe, removing short fibres and neps.
- Detaching and piecing: the nippers open, detaching rollers turn backward to return the previously combed web, which overlaps the new fringe, then turn forward and pull the fringe out; the fibre tails are combed by the top comb as they are drawn through it.
- Noil removal: the combed-out waste is cleaned from the cylinder by a brush and carried away by air.
Production per hour = nips/min × feed per nip × lap tex × heads × (1 − noil fraction) × 60. For 8 heads, 400 nips/min, feed 5 mm per nip, lap 70 ktex (70 g/m) and noil 16 %: lap fed per head per minute = 400 × 0.005 m × 70 g/m = 140 g, so 1120 g/min for 8 heads, 940.8 g/min of combed sliver, which is 56.4 kg/h at 100 % efficiency. Recent developments are higher nip rates with servo drives, lighter moving masses, automatic lap changing and piecing, and individually adjustable noil settings.
Key takeaways
- GOT = lint ÷ seed cotton × 100; the roller gin is gentle on long staple, the saw gin is fast and cuts more fibre.
- Cleaning follows opening; cleaning efficiency = (trash in − trash out) ÷ trash in × 100, and stronger beating adds neps and breaks fibre.
- Carding action is point-against-point between cylinder and flats; settings and wire get finer toward the flats; a periodic fault has wavelength λ = πd × (draft after the faulty roller).
- Open-loop levellers sense the input and act after a delay of distance ÷ speed; closed-loop levellers sense the output and correct their own drift.
- Draft = V_front ÷ V_back; delivered tex = n × feed tex ÷ draft; doubling n independent slivers reduces CV by √n; floating fibres cause drafting waves.
- Combing removes short fibre, neps and trash through feeding, nipping and combing, detaching and piecing, and noil removal; production = nips/min × feed × lap tex × heads × (1 − noil).
Practice questions (17)
Attempt each one before opening the answer. Every explanation names the tempting wrong option as well as the right one, because that is where marks are lost.
Which gin is preferred for long-staple cotton that must be handled gently, and why?
Show answer
Answer: D — Roller gin, because a roller grips the fibre while a knife strips off the seed, damaging the fibre less
The roller gin handles fibres gently and is used for long and extra-long staple, though it is slower. The saw gin is faster but cuts and tangles more fibre, so it suits short and medium staple; it does not lengthen fibre. Out-turn depends mainly on the cotton variety, not on the gin type being the highest.Why can a blowroom not remove trash efficiently from large, tightly compressed tufts?
Show answer
Answer: C — Trash is held inside the tuft, so it can be exposed to the grid bars only after the tuft has been opened
Impurities are embedded in the tufts; cleaning needs opening first, which is why opening is progressive. The tempting alternative about weight is wrong: large tufts are retained by the grid, they do not fall through it.In which arrangement of two wire-covered surfaces does the carding action take place?
Show answer
Answer: D — The points face each other, the surfaces move at different speeds and fibres are held on one and combed by the other
Carding is point-against-point with differing speeds, as between cylinder and flats. The same-direction arrangement described in the first alternative is the stripping action.The cylinder–flats setting of a card is reduced from a wide to a close gauge, all else unchanged. Which outcome is most likely?
Show answer
Answer: A — Carding is more intense and neps removal improves, with more fibre breakage and faster wire wear
A closer gap makes the flats work harder on the fibre fringe, so carding intensity and nep removal rise, at the cost of fibre cutting and wear. Wider settings give the less intense carding named in the first alternative.Which clothing rule is correct for a card?
Show answer
Answer: B — A finer fibre calls for a finer clothing with more points per unit area
Finer fibres need finer, denser wire to be held and opened without being crushed. Sharp teeth are essential, so clothing is ground; flats normally carry flexible clothing, while the taker-in and, on modern cards, cylinder and doffer carry metallic clothing.What distinguishes an open-loop autoleveller from a closed-loop one?
Show answer
Answer: C — The open-loop type senses the input and times its correction for the sensed material, but cannot detect its own errors
Open loop measures before the correction point and therefore needs a timed delay; because the output is not checked, errors it makes itself go unnoticed. Closed loop measures the output and feeds back, so it detects its own drift but corrects material already delivered.What is the main effect of setting the roller gap in a drafting zone smaller than the length of the longest fibres, other things equal?
Show answer
Answer: A — Fibres are gripped by both roller pairs at once, so they break or the rollers slip, spoiling drafting
A fibre longer than the gap is held at both ends, one pair holding it back while the other pulls it forward, so it breaks or slips. Floating fibres are the opposite problem and occur when the gap is too wide.Increasing the noil percentage in combing generally has which combined effect on the combed sliver?
Show answer
Answer: D — Mean fibre length rises and short-fibre content falls
Noil is rich in short fibre and neps, so removing more of it raises mean length and lowers short-fibre content, giving a stronger, more even yarn at a higher cost. Neps fall, not rise, with more combing.A drawframe autoleveller senses the sliver 0.30 m before the point where the main-draft speed is changed. The sliver moves at 15 m/min in that stretch. After how long must the speed change be applied to a sensed thick place so that it acts on that very place?
Show answer
Answer: B — 1.2 s
Delay = distance ÷ speed = 0.30 m ÷ (15 m/min) = 0.02 min = 1.2 s. Using 15 m/s instead of 15 m/min gives 0.02 s; stopping at 0.02 min without converting, or slipping by a factor of ten, gives the other wrong values.Which of the following statements about ginning, opening, cleaning and blending are correct?
Show answer
Answer: A — Ginning out-turn is the lint mass divided by the seed-cotton mass, expressed as a percentage; B — Grid bars let heavy trash fall out while the fibre tufts are carried on; D — Plucking from many bales at once gives bale-to-bale blending
The statements on out-turn, grid bars and multi-bale plucking are correct. Stronger beating also breaks fibre, makes neps and adds short fibre, so the statement that it always improves quality is wrong.Which statements about periodic mass variation and drafting are correct?
Show answer
Answer: A — A fault from an eccentric roller repeats at a wavelength proportional to its circumference and to the draft after it; B — Floating fibres cause drafting waves whose wavelength is related to the fibre length, not to a roller circumference
Mechanical faults give λ = πd × D and drafting waves track fibre length. Doubling n independent slivers lowers the CV by √n, so four slivers halve it. The front delivery roller has no draft after it, so its fault stays at πd.In the cotton combing cycle, which statements are correct?
Show answer
Answer: A — The half-lap of needles combs the fibre fringe while the nippers hold it; B — The top comb combs the tail ends of fibres as the fringe is drawn out during detaching
Combing happens on the fringe held by the nippers, and the top comb treats the rear ends during detaching. Noil is made of short fibres and neps, and the detaching rollers do reverse to return the web for piecing.A card delivers sliver at 120 m/min. The sliver is 4800 tex (g/km). Take the card’s running efficiency as 90 %. The production is ____ kg/h (answer to one decimal place).
Numerical answer — type the value.
Show answer
Answer: 31.1
Delivered length per hour = 120 × 60 = 7200 m = 7.2 km. Mass = 7.2 km × 4800 g/km = 34 560 g = 34.56 kg at 100 %. At 90 %: 34.56 × 0.9 = 31.104, so 31.1 kg/h.Six slivers of 3600 tex are fed to a drawframe whose total draft is 7.5. Ignoring waste, the delivered sliver is ____ tex.
Numerical answer — type the value.
Show answer
Answer: 2880
Delivered tex = n × feed tex ÷ draft = 6 × 3600 ÷ 7.5 = 21 600 ÷ 7.5 = 2880 tex. Forgetting the doubling (3600 ÷ 7.5 = 480) is the usual slip.The back roller of a drafting system has a diameter of 28 mm and has a bent journal that causes one periodic fault per revolution. The total draft between this roller and the delivery is 6. The fault wavelength in the delivered strand is ____ mm (nearest whole number; use π = 3.1416).
Numerical answer — type the value.
Show answer
Answer: 528
Material delivered per revolution = π × 28 = 87.96 mm. After the draft of 6 it is stretched to 87.96 × 6 = 527.8 mm, which is 528 mm.A comber has 8 heads and runs at 400 nips per minute. Each nip feeds 5 mm of a lap of 70 ktex (70 g per metre). Noil is 16 % of the feed mass. At 100 % efficiency the combed-sliver production is ____ kg/h (answer to one decimal place).
Numerical answer — type the value.
Show answer
Answer: 56.4
Lap fed per head per minute = 400 × 0.005 m = 2 m, which is 2 × 70 = 140 g. Eight heads: 1120 g/min. Combed sliver = 1120 × 0.84 = 940.8 g/min = 56 448 g/h = 56.4 kg/h.In a blowroom stage the feed contains 4.0 % trash and the delivered material contains 2.5 % trash. Using cleaning efficiency (%) = (trash % in feed − trash % in delivery) ÷ trash % in feed × 100, the cleaning efficiency is ____ %.
Numerical answer — type the value.
Show answer
Answer: 37.5
(4.0 − 2.5) ÷ 4.0 × 100 = 1.5 ÷ 4.0 × 100 = 37.5 %. Dividing by the delivery trash instead gives 60 %, a common slip.